Problem: Heat Spreader Flatness Fails After Anodize — Mask the Thermal Face

Problem: Al6061 heat spreaders meet thickness in-process, then after clear/black anodize the thermal face bows past 0.05 mm and TIM contact dies.

Root cause: whole-part anodize with no masking; powder coat chosen for cosmetics even though film thickness hurts conduction.

Fix: as-machined thermal face + anodize only non-contact sides; put flatness and cutout tolerances on the PDF; sample flatness before ship.

Lead sketch: Standard ≈ 8–10 days with finish; skip powder on contact plates.

Upload STEP + PDF on the quote page — pick finish carefully, then open the electronics industry page for EMI / cover siblings.

AIkakumafɔlenEmail
PDF

Baara email de ka fisa ([email protected]). Mɔgɔ yɛrɛ ka batakiw bɛ OK. A bɛ se ka kɛ — telesarse bɛ baara kɛ hali bi.

An bɛna baara kɛ ni nin baara imɛri ye dɔrɔn walasa ka nin fɛn in ci ani k’i ka ɛntɛrinɛti ɲininkaliw jaabi (quote, lead time, drawings).

Problem: Heat Spreader Flatness Fails After Anodize — Mask the Thermal Face — Zoryra Precision